The Relationship between Heat Input and Weld Size

Heat input is important because it has an effect on cooling rates which in turn can significantly affect the mechanical properties of the weld and heat affected zone. It also plays a role in susceptibility to distortion.  High heat input can be beneficial in some cases and detrimental in others.  A common misconception is that as long as amperage and voltage remain the same that heat input doesn’t change.  This is wrong because travel speed is also a factor. 

Heat input is a function of three essential variables: amperage, voltage and travel speed.  Change one and heat input changes.  

The formula for heat input is as follows:

HEAT INPUT = (60 x Amps x Volts) / (Travel Speed) =  Joules/Inch

When we keep amperage constant, our deposition rate remains the same.  So in order to make a bigger weld we would have to slow down our travel speed.  If we slow down our travel speed, based on the formula above, our heat input would increase.  Conversely, if we want to make a smaller weld we would need to increase our travel speed, thus decreasing our heat input.  

To illustrate this let’s assume that we have a GMAW welding procedure that calls for the use of .045 ER70S-6 wire to be run at 400 inches/minute (280 amps) and 27.0 volts.   Several fillet welds are to be made. There are a total of 3 different sizes:  3/16-in, ¼-in and 5/32-in.  

At the stated wire feed speed of 400 in/min an .045” solid wire will deposit about 10.5 lb/hr.  At this deposition rate we would need a travel speed of 20 inches per minute to deposit a ¼-inch fillet weld.  

This same deposition rate would require a travel speed of 35 inches per minute to make a 3/16” fillet weld.  And a travel speed of 13 inches per minute to make a 5/16-inch fillet weld. 

At the same wire feeds, and thus same deposition rate, a faster travel speed will yield a smaller weld and lower heat input.

At the same wire feeds, and thus same deposition rate, a faster travel speed will yield a smaller weld and lower heat input.

The resulting heat input to make each of these weld is as follows:

3/16-inch weld = (60 x 280 x 27) / (39) = 11,630 KJ/in

1/4-inch weld = (60 x 280 x 27) / (20) =  22,680 KJ/in

5/16-inch weld (60 x 280 x 27) / (13) =  34,892 KJ/in

* These are approximate weld sizes. Actual sizes are shown in the above image.

This is the reason why AWS D1.1 has minimum fillet weld sizes.   Many incorrectly assume that the minimum sizes have to do with weld strength.   The reason for minimum fillet weld sizes has to do with heat input.  If your heat input gets too low the weld and heat affected zone may cool fast enough to allow the formation of martensite.  This in turn makes the weldment susceptible to hydrogen induced cracking

REFERENCEWelding Procedure Development for Non Welding Engineers


AWS D1.1 Prequalified Welding Procedures

 332 Prequalified Welding Procedure Specifications for Steel Fabricators. Developed and reviewed by welding engineers and certified welding inspectors.

 Find out the details here!

Please note: I reserve the right to delete comments that are offensive or off-topic.

Leave a Reply to Manish Cancel reply

Your email address will not be published. Required fields are marked *

3 thoughts on “The Relationship between Heat Input and Weld Size

  1. Excellent article. Especially the last para where you described why there is a minimum fillet weld size recommended in AWS.

  2. Great article. But why does the smaller, faster weld with the least heat input show the greatest root penetration?

    • Great observation and questions. The deposition rate is very high so a fast travel speed allows the wire to hit the root of the joint and stay ahead of the weld puddle. WHen you slow down the puddle starts to get ahead of the wire and the wire is now driving into the puddle rather than straight into bare metal. If we were to slow down further we would lose penetration into the root and risk lack of fusion.